Konpozisyon

Tablo 1.Ranje konpozisyon pou 316 klas nan asye pur.

Klas CMnSiPSKrMoNiN
316Min---0-16.02.0010.0-
Max0.082.00.750.0450.0318.03.0014.00.10
316LMin-----16.02.0010.0-
Max0.032.00.750.0450.0318.03.0014.00.10
316HMin0.040.040--16.02.0010.0-
max0.100.100.750.0450.0318.03.0014.0-

 

Pwopriyete mekanik

Tablo 2.Pwopriyete mekanik nan 316 klas asye pur.

KlasTensile Str (MPa) minSede Str 0.2% Prèv (MPa) minLong (% nan 50 mm) minDite
Rockwell B (HR B) maxBrinell (HB) max
3165152054095217
316L4851704095217
316H5152054095217

 

Remak: 316H gen tou yon egzijans pou yon gwosè grenn ASTM non . 7 oswa pi grosye.

Pwopriyete Fizik

Tablo 3.Pwopriyete fizik tipik pou asye pur klas 316.

KlasDansite (kg/m3)Modil elastik (GPa)Ko-efè mwayen ekspansyon tèmik (µm/m/°C)Kondiktivite tèmik (W/mK)Espesifik Chalè 0-100 °C (J/kg.K)Rezistans elektrik (nΩ.m)
0-100 °C0-315 °C0-538 °CNan 100 °CNan 500 °C
316/L/H800019315.916.217.516.321.5500740

 

Konparezon Spesifikasyon Klas

Tablo 4.Espesifikasyon klas pou 316 klas asye pur.

KlasUNS NoOld BritanikEuronormSwedish SSJaponè JIS
BSEnNonNon
316S31600316S3158H, 58J1.4401X5CrNiMo17-12-22347SUS 316
316LS31603316S11-1.4404X2CrNiMo17-12-22348SUS 316L
316HS31609316S51-----