Rezistans Kowozyon - 410S

5% Tès
Solisyon nan 120 degre F
(49 degre)

Pousantaj Kowozyon an Mils pa ane ak Milimèt pa ane (mm/a)

Alyaj 409 Alyaj 410S Alyaj 420 Alloy 425 Mod Alyaj 440A Alyaj 430
Asid Acetic 0.88
(0.022)
0.079
(0.002)
1.11
(0.028)
4.79
(0.122)
2.31
(0.0586)
0.025
(0.0006)
Asid fosforik 0.59
(0.002)
0.062
(0.002)
0.068
(0.002)
0.593
(0.015)
0.350
(0.009)
0.029
(0.001)

 

Analiz Chimik

Austenitic Nerjaveèi yo konsidere kòm pi soude nan segondè -aye alyaj yo epi yo ka soude pa tout pwosesis fizyon ak rezistans soude.

       
Kwòm 11.5 min.-14.5 max. Soulf .030 max.
Nikèl 0.60 max. Silisyòm 1.00 max.
Kabòn 0.08 max. Balans*
Manganèz 1.00 max. Fosfò 0.040 max.

 

Pwopriyete mekanik

Tipik Tanperati Chanm Mekanik Pwopriyete, Mill rkwit

Sede fòs
0.2% Offset

Ultim Tensile
Fòs

Elongasyon
nan 2 pous.

Dite
Rockwell B

Rediksyon
pousan nan zòn nan

psi (MPa) psi (MPa)      
42,000 290 64,400 444 33 75 65